| 性能项目 | 试验条件[状态] | 测试方法 | 测试数据 | 数据单位 | ||
| 基本性能 | 密度 | ASTM D-1505 | 0.923 | g/cc | ||
| 熔体流动速率 | ASTM D-1238 | 3.0 | g/10min | |||
| 机械性能 | 下降冲击强度 | ASTM D-1709 | 75 | g | ||
| 延伸率(破断点) | ASTM D638 | 700 | % | |||
| 断裂拉伸强度 | MD | ASTM D-882 | 220 | kg/cm2 | ||
| TD | ASTM D-882 | 190 | kg/cm2 | |||
| 抗张强度(破断点) | ASTM D-638 | 120 | kg/cm2 | |||
| 拉伸抗热强度 | MD | ASTM D-1004 | 95 | kg/cm | ||
| TD | ASTM D-1004 | 90 | kg/cm | |||
| 断裂伸长率 | MD | ASTM D-882 | 350 | % | ||
| TD | ASTM D-882 | 500 | % | |||
| 热性能 | 维卡软化点 | ASTM D-1525 | 88 | ℃ | ||
| 熔点 | ASTM D-2117 | 111 | ℃ | |||
| 其它性能 | 光泽度 | 45 | ASTM D-2457 | 75 | % | |
| 混浊度 | ASTM D-1009 | 6.0 | % | |||
| 厚度 | HCC | 0.03 | ㎜ | |||