| 断裂伸长率 | 600% | 密度 | 0.924g/cm3 | 熔体流动速率 | 0.8g/10min |
| 维卡软化点 | 98℃ | 用途级别 | 薄膜级 | 规格级别 | 薄膜 |
| 缺口冲击强度 | 180 |
|
|
产品简述
| 断裂伸长率 | 600% | 密度 | 0.924g/cm3 | 熔体流动速率 | 0.8g/10min |
| 维卡软化点 | 98℃ | 用途级别 | 薄膜级 | 规格级别 | 薄膜 |
| 缺口冲击强度 | 180 |
详细数据
订购指南
| 性能项目 | 试验条件[状态] | 测试方法 | 测试数据 | 数据单位 | ||
| 其它性能 | 断裂点伸长率 | MD | ASTM D-882B | 380 | % | |
| TD | ASTM D-882B | 600 | % | |||
| 基本性能 | 熔体流动速率 | ASTM D-1238 | 0.8 | g/10min | ||
| 密度 | ASTM D-1505 | 0.924 | g/cm3 | |||
| 物理性能 | 薄膜厚度 | 30-120 | ||||
| 浊度 | ASTM D-1003 | 7.5 | % | |||
| 机械性能 | 断裂点强度 | MD | ASTM D-882B | 220 | kg/cm2 | |
| TD | ASTM D-882B | 190 | kg/cm2 | |||
| 1%伸长弹性系数 | MD | ASTM D-882B | 1900 | kg/cm2 | ||
| TD | ASTM D-882B | 2150 | kg/cm2 | |||
| 落球冲击强度 | ASTM D-1709 | 180 | g | |||
| 降伏点强度 | MD | ASTM D-882B | 100 | kg/cm2 | ||
| TD | ASTM D-882B | 110 | kg/cm2 | |||
| 热性能 | 熔点 | DSC | 114 | ℃ | ||
| 脆化温度 | ASTM D-746 | <-75 | ℃ | |||
| 软化点 | ASTM D-1525 | 98 | ℃ | |||
| 其它性能 | 抗撕裂性 | MD | ASTM D-1922 | 45 | N/mm | |
| TD | ASTM D-1922 | 60 | N/mm | |||
| 光泽度 | 45℃ | ASTM D-2457 | 65 | % | ||
| 摩擦系数 | ASTM D-1894 | 0.11 | ||||