| 断裂伸长率 | 750% | 拉伸强度 | 34MPa | 密度 | 0.92g/cm3 |
| 熔体流动速率 | 1g/10min | 用途级别 | 薄膜级 | 规格级别 | 薄膜 |
| 脆化温度 | -70℃ | 特性级别 | 透明级,热稳定性,高光泽 |
|
|
产品简述
| 断裂伸长率 | 750% | 拉伸强度 | 34MPa | 密度 | 0.92g/cm3 |
| 熔体流动速率 | 1g/10min | 用途级别 | 薄膜级 | 规格级别 | 薄膜 |
| 脆化温度 | -70℃ | 特性级别 | 透明级,热稳定性,高光泽 |
详细数据
订购指南
| 性能项目 | 试验条件[状态] | 测试方法 | 测试数据 | 数据单位 | ||
| 基本性能 | 熔体流动速率 | ASTM D-1238 | 1.00 | g/10min | ||
| 密度 | ASTM D-1505 | 0.920 | g/cm3 | |||
| 物理性能 | 薄膜厚度 | HYUNDAI | 30 | um | ||
| 光泽度 | 45℃ | ASTM D-2457 | 60 | |||
| 机械性能 | 撕裂拉伸强度 | MD | ASTM D-882 | 450 | kg/cm2 | |
| TD | ASTM D-882 | 350 | kg/cm2 | |||
| 撕裂伸长 | MD | ASTM D-882 | 600 | % | ||
| TD | ASTM D-882 | 750 | % | |||
| 落球冲击强度 | ASTM D-1709 | 80 | g | |||
| 撕裂强度 | MD | TEAR LENGTH 21.5mm | ASTM D-1992 | 500 | % | |
| TD | TEAR LENGTH 21.5mm | ASTM D-1992 | 150 | % | ||
| 热性能 | 低温脆点 | ASTM D-746 | <-70 | ℃ | ||
| 其它性能 | 雾度 | ASTM D-1003 | 14 | % | ||